Stainless seat pans: blank size, draw limits, springback and the checking fixture that keeps 500 pans in one shape

The pressed stainless seat pan never comes out of the die at the angle the die was cut to. Springback of 3 to 5 degrees on a flange and 8 to 12 percent on a 40 mm draw is normal material behaviour, and every pan we ship is built around it. This is the blank, clearance, overbend and inspection routine behind that.

Published by JPChairs · Chair manufacturer in Foshan, China · 2026-11-10

Springback is a material number, not a die fault

304 in 1.2 mm sheet runs a yield strength of 205 to 250 MPa, a strain hardening exponent near 0.45 and a modulus of 193 GPa. Bend a flange 90 degrees and it springs back 3 to 5 degrees when the punch lifts. Draw a 40 mm pan and the wall comes back 8 to 12 percent shallower than the die, which is 3.2 to 4.8 mm on that depth. Extra press tonnage does not remove this, it is stored elastic energy coming back out of the part.

Austenitic grades make it worse the second time. A pan pressed from annealed sheet at 205 MPa comes out with 250 to 290 MPa on the worked wall, so a re-strike springs back less, not more. When a shop says the second hit fixed the shape, they changed the part rather than the material.

Blank size and how far a pan can be drawn

The 430 by 430 mm pan with a 40 mm wall and a 30 mm corner radius needs a 470 by 470 mm blank, a blank to draw ratio near 1.09. Past 1.25 the wall thins beyond 20 percent and the corners tear, so anything deeper than 55 mm on 1.2 mm sheet goes to two draws with an interstage anneal at 1,050 C.

Thinning is the number to watch at first article. The worst point sits where the wall meets the floor at the corner: at 1.2 mm nominal we accept down to 0.96 mm, and 0.90 mm or below is a reject even before it cracks, because it will crack at the weld in service.

Die clearance and the overbend routine

Clearance is 8 to 10 percent of thickness, so 0.10 to 0.12 mm per side on 1.2 mm sheet. At 5 percent the sheet galls and picks up die material, and every fourth or fifth part carries a scratch that costs 45 to 60 seconds of polishing to clear.

We cut the die 3 to 5 degrees past 90 and 2 to 3 mm over on wall height, then adjust by 0.3 to 0.5 mm per trial. Three trials is normal to hold a 1.0 mm form gauge, and the fourth catches batch drift once the die has run 20,000 hits. Dies are Cr12MoV on a 100 to 160 tonne press, polished at 50,000 hits and rebuilt at 200,000.

Surface defects and what actually causes them

Orange peel means the grain is too coarse: anything above 40 microns shows as a stipple at 1.2 mm and no polish hides it, so the coil goes back for a 1,050 C solution anneal and a 2B finish at Ra 0.4 microns. Stretcher strains show on 201 and rarely on 304, one more reason the two grades are not interchangeable on a visible seat pan.

Die marks fail at 0.02 mm depth under 500 lux at 500 mm. Removal runs 240 grit across the mark, then 320 grit along the grain to match the No.4 direction, and the whole face is re-grained because a local patch shows at an 8 degree viewing angle.

The checking fixture and the sampling plan

Each pan model gets a fixture with 12 locating stops. Six gap checks must read 1.0 mm or under, the diagonal is held to plus or minus 1.5 mm, and flatness across 430 mm to 1.5 mm. The first three pans off a new die go to a full dimensional report, then it is 1 in 200, plus five parts after every die service.

After the pan is spot welded to the frame at four points the seat height is re-checked, because 1.2 mm sheet pulls 0.5 to 1.0 mm at each weld and four welds put 2 mm of bow into a flat pan.

Fixtures wear as well. The 12 stops in a hard anodised checking fixture lose about 0.05 mm every 15,000 pans, so the fixture is verified against a master pan on the first shift of each week and reset when any stop reads 0.10 mm out. A fixture drifting out of spec is worse than none, because it passes parts that the customer jig will reject and the complaint lands at the dock.

Cost per pan and when to stop pressing

The 430 mm pan die costs 3,000 to 6,000 USD. Amortised over 5,000 pans that is 0.60 to 1.20 USD per part, on top of a 6 to 8 second press cycle, 25 to 35 seconds of deburring and 45 to 60 seconds of grain matching. Below roughly 300 pans a year the die never pays back, and a frame welded from 0.9 mm flat sheet at 12 to 18 minutes per unit is cheaper and just as strong.

Lead time moves with the tooling decision too. A welded frame trial of 300 pans ships in 25 to 30 days from drawing approval, while a new die adds 20 to 25 working days of build and trials before the first good pan comes off the press.

The stainless steel chairs with pressed seat pans we build are quoted with die amortisation as a separate line, so a repeat order at 5,000 pieces drops the unit price visibly. The press and fixture side of the shop is set out on our factory press forming shop page.

Questions buyers ask

FAQ

How much springback should I expect on a 304 seat pan?

8 to 12 percent of draw depth, so 3.2 to 4.8 mm on a 40 mm pan, plus 3 to 5 degrees on any 90 degree flange; the die has to be cut over size to land on nominal.

Why do pressed pans crack at the corner radius?

An inner radius under 1t with wall thinning past 20 percent. Hold the corner at 1.5t, which is 1.8 mm on 1.2 mm sheet, and keep the blank to draw ratio under 1.25.

How many pans before a press die needs service?

Polish at 50,000 hits and rebuild at 200,000 on a Cr12MoV die, with a 1 in 200 dimensional check and five parts inspected after every service.