Cut edges on stainless chair tubes decide the weld
Most stainless chair problems we are asked to trace do not start at the welding torch. They start at the laser, on a cut face nobody photographed and nobody measured.
Published by JPChairs · Chair manufacturer in Foshan, China · 2026-11-18
Where the cut edge decides the outcome
The cut end of a tube fixes three things downstream: how tight the joint closes before welding, how much polishing the frame needs afterwards, and how long the surface survives in a wet kitchen. On a 1.5 mm wall 304 tube, a cut that is square within 0.1 mm closes to a gap under 0.15 mm, which is the range our TIG welders fuse without filler rod. A cut that is 0.3 mm out of square leaves a gap the welder fills with rod, and filler on thin wall means more heat, more distortion and a weld toe that has to be ground back later.
- Wall thickness 1.2 to 2.0 mm covers most frames; the shop runs 1.5 mm as standard for legs and 1.2 mm for back hoops.
- Squareness target is 0.3 mm per 100 mm of cut, checked with a machinist square and a 0.1 mm feeler at four points around the tube.
- Burr above 0.1 mm is a cut finger at packing, so every end is deburred before welding rather than after.
Kerf, speed and assist gas on thin wall
Fiber laser at 1.5 to 3 kW cuts 304 tube cleanly when gas and speed are matched to the wall. We cut 1.5 mm with nitrogen at 12 to 16 bar and 3 to 5 m/min, giving a kerf of 0.15 to 0.25 mm. Cutting the same wall with oxygen runs faster on thicker sections but leaves a heavier oxide on the cut face and a wider heat affected zone, which costs polishing time later.
- Focus sits 0 to -1 mm below the surface on 1.2 to 1.5 mm wall; going deeper narrows the kerf and raises dross on the underside.
- Nozzle 1.5 to 2.0 mm single orifice, changed when the bore shows spatter build-up, typically every 40 to 60 cutting hours.
- Length tolerance ±0.1 mm on a programmed part, hole position ±0.2 mm, which is what the M8 weld nuts on seat rails need.
- Cut face angularity held under 0.05 mm across a 1.5 mm wall, measured on a profile projector at 20x.
Dross and heat tint before welding
Dross on the underside of a cut is not cosmetic. Beads of 0.1 to 0.3 mm sit exactly where the two parts have to meet, so the welder either grinds them off and loses the square edge, or clamps the joint over them and welds a gap. Heat tint is worse: it is a chromium-depleted layer 0.05 to 0.2 um thick. Left in place, salt spray shows red rust at 96 to 168 hours on a part that should pass 480 hours.
- Hand deburr on a linisher with 120 to 180 grit takes 20 to 40 seconds per cut end; 30 to 45 cut ends per chair adds 15 to 25 minutes of labour.
- Pickling paste or bath for 20 to 30 minutes at ambient, then citric passivation at 60 C for 10 minutes, restores the passive layer on the cut face.
- Carbon steel wire brushes transfer free iron and produce rust spots within days; stainless brushes only, kept for stainless work.
Fit-up numbers the welder works to
Every welder on stainless tube works inside a gap window. Ours is 0 to 0.15 mm on a butt joint at 1.5 mm wall, with mismatch capped at 0.2 mm, about 13% of the wall. Past 0.3 mm of gap the joint needs filler wire, welding speed drops roughly 30%, and shrinkage on an eight-joint frame doubles from 0.5 to 1.0 mm per joint, which is 4 to 8 mm across the whole frame.
- Tack welds 4 to 6 mm long, placed opposite each other, 5 to 8 mm in from the joint end.
- Purge or backing gas on closed sections; sugar on the inside of a tube becomes a corrosion cell nobody can reach again.
- Weld toe is ground flush on A faces only. Removing 0.1 mm from a 1.5 mm wall is 7% of the section on a part already at its design limit.
Nesting, cut length and cost per chair
One stainless dining chair carries 6.5 to 8.5 m of cut tube across 30 to 45 cuts. Bars arrive in 6 m lengths, and nesting at 84 to 89% yield leaves 2 to 4% offcut scrap that goes back as rems for small brackets. Laser time lands at 0.35 to 0.60 USD per chair and deburring at 0.25 to 0.35 USD, which is small against the welding hours but visible on a 500 chair order.
- Shared cut lines between two parts on the same bar save one kerf and one pierce: 0.2 mm of material and about 0.8 seconds each.
- Common-line nesting on the four legs of one chair returns 3 to 5% material on a 6 m bar.
- Batches of 200 chairs per size and colour keep bars inside one nesting run instead of re-setting between orders.
Incoming checks on cut parts
Cut parts are inspected before they reach the welding fixture, because a fixture clamps a bad cut into a bad frame and the defect is then locked in by six welds. The checks are simple enough to run at the machine, which is where they have to happen.
- First-off inspection of 5 pieces per program: length, squareness, burr, dross and angularity recorded on the route sheet.
- Then 1 piece per 50, with calipers and square kept at the laser rather than in the QC office.
- Rework limit: a cut end 0.2 mm long can be linished back; anything short of nominal is scrap, because welding cannot add length.
- Salt spray coupons from each batch: 480 hours on 304 with pickled cut faces, 96 to 168 hours when the oxide is left on.
- The laser-cut stainless steel chairs we ship are built to these cut and fit-up windows, and the factory laser tube cutting cell holds them on 304 and 316L on the same program.