What eight welds do to a square frame
The four-leg iron chair carries six to nine fillet welds, and each one pulls as the bead cools and shrinks. The fixture holds most of that back, but the release always leaves something behind.
- Typical post-weld errors are 2 to 4 mm of leg splay at the floor, a 1 to 3 mm difference in seat height corner to corner, and 1 to 2 mm of twist across a 400 mm diagonal.
- Our acceptance gates are a 0.5 mm feeler under any foot on the granite table, seat height within 2 mm of nominal, and no visible twist over a 500 mm diagonal check.
- Small frames forgive; a 760 mm high-back frame does not, because 3 mm of splay at the floor becomes 8 mm at the top rail and the chair visibly leans on a flat floor.
- Distortion is measured before grinding, since grinding a weld that will be straightened afterwards just doubles the handling.
Cold straightening at the press
Most corrections are cold, on a 16 to 20 tonne hydraulic press with nylon pads and a 150 mm support span.
- Carbon steel springs back 25 to 35 percent of the bend, so the press over-bends 1.3 to 1.5 times the measured error and then re-checks against the gauge.
- The limit is two correction cycles at the same location. Work hardening from the first bend raises local hardness 10 to 15 percent and turns the leg into a fatigue notch exactly where guests rock the chair.
- The single press pass corrects 4 to 6 mm at the leg tip measured over 300 mm; beyond that it is a fixture conversation, not a press conversation.
- Corrections go on legs and rails only, never across a weld toe, where the bend opens the weld root.
Flame straightening, where carbon steel wins
Heat correction is the option carbon steel has and 304 stainless does not, and it saves frames the press cannot reach.
- We heat to 600 to 650 C, a dark cherry colour safely below the 723 C transformation point, in a vee pattern on the outside of the bow.
- Each vee heat pulls 0.4 to 0.8 mm of shrink as it cools, and one spot takes two to three heats at most before the zone is spent.
- Air cooling is standard; a water quench roughly doubles the pull but hardens the zone, so we quench only on thick base metal away from welds.
- Above 700 C the grain grows and the tube surface suffers; on 304 stainless the same operation is simply forbidden, which is why that production line runs cold straightening only.
Back into the gauge before packing
The corrected frame is an unverified frame until it has been through the fixture gauge again.
- Every straightened frame re-runs the pin drop test and the 0.5 mm feeler check on all four feet.
- Welds inside a straightened zone get a dye penetrant check when the tube wall is under 1.5 mm, because a hidden root crack at a bend fails in service within months.
- The coating is repaired where press pads touched: 60 to 80 micron zinc-rich primer followed by powder touch-up, keeping total film above 80 micron at the repair spot.
- Frames that pass return to the stack; frames that fail a second time go to the scrap decision instead of a third bend.
When to scrap instead of fix
Some frames cost more to save than to melt, and the criteria are written down so nobody argues at the bench.
- Scrap when ovality on a 25 mm tube exceeds 1.5 mm, when the wall has thinned below 1.2 mm, when a crack shows at any weld toe, or when a frame needs more than three separate correction points.
- The tube steel in one frame is worth 1.30 to 1.90 USD; three corrections at 3 to 6 minutes each already costs more in labour than the tube does.
- The 1 to 2 percent straightening-driven scrap rate is normal; above 3 percent the fixture needs re-cutting, and blaming the welders will not fix it.
What the buyer puts on the drawing
Straightening is invisible from the outside, so it has to be specified rather than assumed.
- The tolerance list: 0.5 mm feeler under feet, seat height within 2 mm, no twist over a 500 mm diagonal.
- The correction cycle limit of two per location, and a penetrant rule for straightened zones on thin-wall tube.
- The written scrap decision rule, so corrections stop before the steel is damaged further.
Frames built this way go through the post-weld inspection workflow before coating, and the finished iron restaurant chairs held to gauge tolerance are what that bench work is really paying for.