Electropolishing stainless chair frames: removal, Ra and cost
Electropolishing is not a brighter version of buffing. It dissolves metal anodically in a phosphoric and sulphuric acid bath, levelling the micro-profile instead of smearing it, and the difference shows up in salt spray hours rather than in the showroom.
Published by JPChairs · Chair manufacturer in Foshan, China · 2026-11-20
What the bath removes, in microns
The bath runs 60 percent phosphoric and 40 percent sulphuric acid by volume, at 45 to 60 C, with 12 to 25 A per square decimetre of wetted surface. Immersion runs 3 to 8 minutes and removes 5 to 15 microns per exposed face, which is enough to flatten the peaks left by 180 or 240 grit belt work.
- Surface roughness falls from Ra 0.6 to 0.8 microns after belt polishing to Ra 0.20 to 0.35 microns after electropolishing.
- Gloss rises to 350 to 600 gloss units at 60 degrees, brighter than a No.4 brushed finish at 120 to 160 GU and duller than a mirror buff at 700 GU and above.
- Current is sized on the part, not on the rack: a chair frame has 2.4 to 2.8 m2 of wetted area, so a six-frame rack at 18 A/dm2 draws about 280 A from the rectifier.
- Bath temperature below 40 C slows levelling and leaves a milky bloom; above 65 C the acid attacks fixture contacts and erodes the tank lining.
Why buffing is not a substitute
Mechanical polishing folds metal over instead of removing the damaged layer. The result looks right for a week, then free iron left in the surface and polishing compound trapped in crevices start to work, and the first rust bloom appears where a buyer photographs the weld.
- Buffed 304 tested to ASTM B117 typically shows rust at 96 to 168 hours. Electropolished 304 of the same grade reaches 480 hours clean in our records.
- Compound residue sits in the 0.1 to 0.3 mm gap at a welded joint. Electropolishing removes the surface that holds it only if the joint is already closed.
- Tube interiors cannot be buffed at all. Electropolishing reaches 300 to 400 mm into a 25 mm tube on the strength of its throwing power, which matters for frames that will see wash-down water.
- Labour is the other half: buffing a chair frame takes 35 to 50 minutes by hand, electropolishing is 6 to 10 minutes of racking plus bath time.
Racking, contact marks and current distribution
Every part must be electrically connected, and every contact point is a place the process cannot polish. We rack on hidden surfaces, inside a leg pocket or under a seat pan, and cap the contact at 3 to 5 mm diameter.
- Spring clips at 15 to 25 N hold the frame without arcing; a loose clip burns a 0.5 to 1.0 mm pit that cannot be polished out.
- Three to four contacts per frame, spread so no single contact carries more than 40 percent of the current.
- Current density varies 20 to 30 percent between the end nearest the bus bar and the far end of a 2,800 mm rack, which shows as a 2 to 4 GU gloss difference. Rotating rack position each cycle evens it out.
- Titanium racks last 3 to 5 years in this bath; copper or brass racks contaminate the acid with 50 to 200 ppm and cause copper plating on the parts.
What it does not fix
Electropolishing is a surface process, and 15 microns of removal cannot rescue a bad weld or a coarse scratch. It also has side effects on edges and threads that drawings rarely mention.
- Weld toes are rounded and porosity is opened rather than closed. A 0.3 mm pit becomes a 0.32 mm pit with a cleaner rim and a visible ring.
- Edges round by 0.02 to 0.05 mm per 10 microns removed. On a laser-cut edge this reads as a soft line, which is fine on a seat pan and wrong on a visible 1.2 mm plate edge that should stay crisp.
- Wall loss is real: 15 microns per face on a 1.2 mm tube is 1.25 percent of wall, so a 1.0 mm minimum wall drawing must start at 1.05 mm.
- Threads need masking plugs; an unmasked M6 thread grows 0.02 to 0.04 mm across the flanks and will not take a nut. Holes open by 0.01 to 0.02 mm per side.
- Assemblies with brass inserts, zinc-plated springs or carbon steel fasteners cannot go in the bath at all, because the zinc and iron dissolve and plate out on the stainless.
Acceptance on the shop floor
Our acceptance sheet is three measurements plus a coupon per batch. Roughness is read at three points per frame, gloss at two, and the coupon goes into salt spray alongside the production lot.
- Ra 0.20 to 0.35 microns on visible faces, Ra 0.45 maximum inside leg pockets, measured with a portable stylus at 0.8 mm cut-off.
- Gloss 350 to 600 GU at 60 degrees, with 40 GU maximum spread across one frame.
- 50 x 50 mm coupon per batch in ASTM B117: 480 hours, no rust at the cut edge or the bend.
- Weight loss 5 to 15 g/m2 on the coupon confirms the removal was inside the booked window; below 5 g/m2 means the rack was underpowered.
- Water break test on a rinsed frame: a continuous film for 30 seconds means the surface is clean and active. Beading means residue, and residue means a re-clean and re-rack.
- Visual check at 500 to 750 lux under 15 degree raking light, 600 mm working distance, with the part held so the light runs along the length.
Cost, capacity and when to skip it
The bath is a fixed cost, so electropolishing only works at volume. A 4,000 litre line runs 120 to 180 chair frames a day in two shifts and needs 30 to 45 minutes of chemistry checks per shift: acid strength, specific gravity at 1.55 to 1.65, aluminium and iron build-up, and temperature.
- Cost per frame at 500 units: 4.20 to 7.50 USD, including racking labour, chemistry drag-out and the 1 to 3 percent rework rate.
- Hand buffing on the same frame runs 2.20 to 3.40 USD, but the rework rate for rust complaints is 4 to 6 times higher and a return shipment costs more than the finish.
- Skip it for powder-coated frames, hidden structural parts, and any frame where the visible edge must stay sharp; a No.4 brushed finish at 120 to 160 GU is the right answer there.
- The finish is worth its cost on bar fronts, open kitchens and wash-down areas, which is why most of the electropolished stainless steel restaurant chairs we ship go to those three applications.